⚡ TL;DR(Too Long; Didn't Read)

Results: Mean :|: standard deviation of SBS values in the control group was 13.42 :I:] .23 Wa and 8.47 i0. 71 MPa in the Er: YAG group and this diflerence was statistically significant (p

📌 3 Key Takeaways

🎯
Objective & Hypothesis:Purpose: The objective of the present study is to evaluate the eflects of Er:YAG laser debonding of ceramic brackets on the bond strength and the amount of adhesive resin remnant.
📊
Key Findings & Data:Materials and Methods: Twenty human mandibular incisors were randomly divided into two groups of 10 andpolycrystalline ceramic brackets (Transcend series 6000, 3M Unitek, Monrovia, CA, USA) were bonded on enamel surfaces.
💡
Conclusion & Impact:Results: Mean :|: standard deviation of SBS values in the control group was 13.42 :I:] .23 Wa and 8.47 i0. 71 MPa in the Er: YAG group and this diflerence was statistically significant (p
🔬Design:Research Article
📍Scope:Comprehensive Sample
⚙️Variables:Domain Parameters

Abstract

Purpose: The objective of the present study is to evaluate the eflects of Er:YAG laser debonding of ceramic brackets on the bond strength and the amount of adhesive resin remnant. Materials and Methods: Twenty human mandibular incisors were randomly divided into two groups of 10 andpolycrystalline ceramic brackets (Transcend series 6000, 3M Unitek, Monrovia, CA, USA) were bonded on enamel surfaces. Group was the control group in which no laser application was performed prior to the shear bond strength (SBS) testing. In Group 2, Er.'YAG was applied in 3W power for seconds using the scanning method. The brackets were testedfor SBS with an Instron universal testing machine and results were expressed in megapascals (Wa). The amount of adhesive remnant was evaluated with Adhesive Remnant Index (ARI). One—way analysis of variance and ukeyîs post-hoc tests were used for statistical analysis. Results: Mean :|: standard deviation of SBS values in the control group was 13.42 :I:] .23 Wa and 8.47 i0. 71 MPa in the Er: YAG group and this diflerence was statistically significant (p

Özet

Amaç: Bu çalışmanın amacı seramik braketlerin Er: YAG lazer ile sökümünün bağlanma dayanımı ve artık adezif rezin miktarı üzerindeki etkilerini değerlendirmektir. Gereç ve Yöntem: Yirmi adet insan alt kesici dişi rastgele olarak eşit sayıda numune içeren iki gruba ayrıldı. Polikristalin seramik braketler (Transcend series 6000, 3M Unitek, Monrovia, CA, USA) dişlerin mine yüzeylerine yapıştırıldı. 1. grup kontrol grubu olup, makaslama bağlanma dayanımı (ABD) testinden önce lazer uygulaması yapılmadı. 2. Gruptaki numunelere gücündeki Er:YAG lazer tarama metoduyla saniye uygulandı. Bütün braketlerin MBD değerleri Instron cihazında ölçüldü ve ölçü birimi megapascal (MPa) olarak ifade edildi. Ayrıca, ArtıkAdezifİndeksi (AAİ) skorları hesaplandı. İstatistiksel analiz için tek yönlü varyans analizi ve post hoc ukey testleri kullanıldı. Bulgular: Her bir grup için ortalama SBS değerleri; kontrol grubunda 13.42 :I:] .23 MPa, Er:YAG lazer uygulanan grupta 8.4 :|:0. 71 Wa olarak ölçüldü. Bu farkın istatistiksel olarak anlamlı olduğu belirlendi (p

🔖

Cite This Article

ERŞAHAN, Ş., ERTÜRK, E., ALAKUŞ-SABUNCUOĞLU, F. I. (2022). DEBONDIN OF CERAMIC BRACKETS BYER:K4G LASER. Journal of Istanbul University Faculty of Dentistry, Cilt: 50 - Sayı: 2, 29–35. https://ajindex.com/articles/563823

📄 Full Text PDF Viewer

📄

PDF görüntüleyici hazırlanıyor...

References (4)

  1. Azzeh E, Feldon PJ. Laser debonding of ceramic brackets: comprehensive review. Am Orthod Dentofacial Orthop 2003; 123(1):79-83
  2. Bishara SE, Trulove TS. Comparisons of different debonding techniques for ceramic brackets: An in vitro study. Part i. Background and methods. Am Orthod Dentofacial Orthop 1990;98(2):145- 153
  3. Eliades T, Eliades G, Brantley WA. Orthodontic brackets. In: Brantley WA, Eliades T, eds. Orthodontic Materials Scientific and Clinical Aspects. Stuttgart, Germany: Thieme; 2001.p.143—72
  4. Macri RT, de Lima FA, Bachmann L, Galo R,. Romano FL, Borsatto MC, Matsumoto MA. C02 laser as auxiliary in the debonding of ceramic brackets. Lasers Med Sci 2015;30(7):1835-1841. Saito A, Namura Y, Isokawa K, Shimizu N. C02 laser debonding of ceramic bracket bonded with orthodontic adhesive containing thermal expansion microcapsules. Lasers Med Sci 2015;30(2):869-874. Ma T, Marangoni RD, Flint W. In vitro comparison of debonding force and intrapulpal temperature changes during ceramic orthodontic bracket removal using carbon dioxide laser. Am Orthod Dentofacial Orthop 1997;111(2):203- 210. Mimura H, Deguchi T, Obata A, Yamagishi T, Ito M. Comparison of different bonding materials for laser debonding. Am Orthod Dentofacial Orthop 1995;108(3):267-273. Obata A, Tsumura T, Niwa K, Ashizawa Y, Deguchi T, Ito M. Super pulse c02 laser for bracket bonding and debonding. Eur Orthod 1999;21(2):193-198. Strobl K, Bahns TL, Willham L, Bishara SE, Stwalley WC. Laser-aided debonding of orthodontic ceramic brackets. Am Orthod Dentofacial Orthop 1992; 101(2):152-15 8. Hayakawa K. Nd: Yag laser for debonding ceramic orthodontic brackets. Am Orthod Dentofacial Orthop 2005;128(5):638-647. Mundethu AR, Gutknecht N, Franzen R. Rapid debonding ofpolycrystalline ceramic orthodontic brackets with an erzYag laser: An in vitro study. Lasers Med Sci 2014;29(5):1551-1556. Oztoprak MO, Nalbantgil D, Erdem AS, Tozlu M, Arun T. Debonding of ceramic brackets by new scanning laser method. Am Orthod Dentofacial Orthop 2010; 13 8(2): 195-200. Reynolds IR. review of direct orthodontic bonding. Br Orthod 1975;2(3):171-178. Gwinnett AJ. comparison of shear bond strengths of metal and ceramic brackets. Am Orthod Dentofacial Orthop 1988;93(4):346-348. Joseph VP, Rossouw E. The shear bond strengths of stainless steel and ceramic brackets used with chemically and light-activated composite resins. Am Orthod Dentofacial Orthop 1990;97(2):121- 125. Tocchio RM, Williams PT, Mayer FJ, Standi