Journals / Turkish Journal of Physics / 2001 / Cilt: 25 - Sayı: 6
Directional solidification of pure succinonitrile and succinonitrile-salol alloys
- Journal
- Turkish Journal of Physics
- Pages
- 563–574
- DOI
- —
Özet
Pure succinonitrile (SCN) and succinonitrile-salol alloys with four different concentrations of salol were unidirectionally solidified at five different growth rates in a temperature gradient. The microstructure parameters, viz., the primary dendrite arm spacing $\lambda_1$, dendrite tip radius R and mushy zone depth d, were measured. The dependence of the microstructure parameters on the solidification parameters for pure SCN and SCN-Salol alloys were determined via linear regression analysis. The results are compared with published data.